CHEMVEN

Spectrophotometric Determination of Manganese in Steel as Permanganate via Periodate Oxidation

To determine the percentage of manganese in a carbon or alloy steel sample by dissolving the alloy in acid, oxidizing manganese(II) quantitatively to intensely purple permanganate, MnO4-, using potassium periodate, and measuring absorbance at 525 nm.

Level: University PracticalSafety: Corrosive / Strong OxidantTime: 90 min
Aim of Experiment: To determine the percentage of manganese in a carbon or alloy steel sample by dissolving the alloy in acid, oxidizing manganese(II) quantitatively to intensely purple permanganate, MnO4-, using potassium periodate, and measuring absorbance at 525 nm.

Theoretical Foundations

Manganese in steel is dissolved in dilute nitric acid and phosphoric acid. Phosphoric acid complexes iron(III) as colorless [Fe(PO4)2]3-, preventing interference from yellow/brown iron(III) ions. Manganese(II) is oxidised quantitatively to purple permanganate (Mn(VII)) by potassium periodate (KIO4) in boiling solution: 2Mn2+ + 5IO4- + 3H2O -> 2MnO4- + 5IO3- + 6H+. Potassium periodate is an ideal oxidant because its reduction product, iodate (IO3-), does not absorb visible light, and periodate does not oxidise chloride to chlorine under these conditions. Permanganate exhibits characteristic vibronic absorption bands with a primary absorption maximum at 525 nm (epsilon ≈ 2,400 L·mol^-1·cm^-1) and follows Beer's law up to 25 mg/L Mn.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Visible spectrophotometer (400-700 nm)
  • 1.00 cm matched glass or quartz cuvettes
  • 250 mL conical flasks
  • 100 mL volumetric flasks
  • Hotplate
  • Analytical balance (±0.0001 g)

Chemical Reagents

  • Steel sample turnings (standard reference material or unknown)
  • Nitric acid (HNO3, 1:3 v/v, 25 mL)
  • Phosphoric acid (H3PO4, 85%, 10 mL)
  • Potassium periodate (KIO4, AR grade crystals)
  • Potassium permanganate standard solution (100 mg/L Mn)
  • Sodium nitrite (NaNO2, 5% w/v, blanking bleach)
  • Deionised water

Step-by-Step Practical Procedure

  1. Weigh accurately about 0.50 g of steel turnings into a 250 mL conical flask.
  2. Add 25 mL of 1:3 nitric acid; heat gently on a hotplate in a fume hood until completely dissolved and brown nitrogen dioxide fumes cease.
  3. Add 10 mL of 85% phosphoric acid; boil for 2 minutes to complex iron(III).
  4. Add approximately 0.5 g of potassium periodate crystals and a few boiling stones.
  5. Boil the solution gently for 5 minutes; observe the development of the characteristic deep purple permanganate color.
  6. Cool to room temperature, transfer quantitatively to a 100 mL volumetric flask, dilute to the mark with deionised water, and mix thoroughly.
  7. Prepare a series of manganese standards (0.0, 2.0, 5.0, 10.0, 15.0, 20.0 mg/L Mn) treated identically with periodate.
  8. Measure the absorbance of the standards and sample at 525 nm using deionised water to zero the instrument.
  9. To prepare the sample blank, add 1 drop of 5% NaNO2 to 10 mL of the sample solution (which instantly bleaches permanganate to colorless Mn2+), and measure its background absorbance; subtract this blank from the sample absorbance.
  10. Calculate the percentage of manganese in the original steel alloy.

Observations & Expected Results

Upon heating with KIO4, the pale yellowish-green solution turns rapidly into an intense, brilliant violet-purple color identical to KMnO4. The addition of a drop of NaNO2 to the blank aliquot discharges the purple color instantly to crystal clear, confirming quantitative bleach.

Worked Stoichiometric Calculations

Problem: 0.5000 g of steel was dissolved, oxidised with KIO4, and diluted to 100.0 mL. Corrected absorbance at 525 nm was A = 0.485. The calibration curve slope was m = 0.0438 L/mg Mn. Calculate the percentage of manganese in the steel sample.

Working: Concentration of Mn in flask C = A / m = 0.485 / 0.0438 = 11.07 mg/L Mn. Total mass of Mn in 100 mL (0.100 L) = 11.07 mg/L × 0.100 L = 1.107 mg = 0.001107 g Mn. Percentage of Mn in steel = (Mass of Mn / Mass of steel sample) × 100 = (0.001107 g / 0.5000 g) × 100 = 0.221% Mn.

Safety Precautions & Hazard Control

  • Use phosphoric acid to completely bleach iron(III); uncomplexed Fe3+ absorbs strongly below 500 nm and causes severe positive bias.
  • Ensure complete removal of nitrogen oxides (NO2) before adding periodate, as nitrites reduce periodate and consume oxidant.

Waste Disposal Protocol

Used permanganate and acid solutions must be treated with sodium bisulphite until colorless and disposed of in heavy metal acidic waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is potassium periodate (KIO4) preferred over potassium persulphate or sodium bismuthate?

A: Periodate oxidises Mn(II) to Mn(VII) cleanly and quantitatively in boiling homogeneous solution; excess periodate and its reduction product (iodate, IO3-) are completely colorless and do not interfere at 525 nm, whereas bismuthate requires filtration and persulphate requires toxic silver catalyst.

Q: Why is phosphoric acid added during steel dissolution?

A: Phosphoric acid performs two vital roles: (1) it forms a stable, colorless complex [Fe(PO4)2]3- with Fe(III), eliminating optical interference at 525 nm; (2) it stabilizes the permanganate color against thermal decomposition.

← Back to Experiments Directory