CHEMVEN

Chromium in Stainless Steel as Barium Chromate

Determine chromium in steel by oxidation to chromate and precipitation as BaCrO4.

Level: UniversitySafety: Advanced lab onlyTime: 4 h
Aim of Experiment: Determine chromium in steel by oxidation to chromate and precipitation as BaCrO4.

Theoretical Foundations

Chromium is oxidised to Cr(VI) with persulfate: 2Cr3+ + 3S2O8 2- + 7H2O → Cr2O7 2- + 6SO4 2- + 14H+. In acetate-buffered solution, barium precipitates the chromate: Ba2+ + CrO4 2- → BaCrO4(s). The bright yellow precipitate is stoichiometric after drying at 150 C. GF for chromium = M_Cr/M_BaCrO4 = 52.00/253.33 = 0.2053.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 400 mL beaker
  • Hot plate
  • Fume cupboard
  • Sintered-glass crucible
  • Oven at 150 C
  • Desiccator

Chemical Reagents

  • Steel sample
  • Sulfuric acid, dilute
  • Ammonium persulfate, solid
  • Sodium acetate buffer
  • Barium chloride solution, 10%
  • Distilled water
  • Cr(VI) PPE (gloves)

Step-by-Step Practical Procedure

  1. Weigh accurately 1.0 g steel; dissolve in 20 mL dilute H2SO4 with warming.
  2. Oxidise: add 2 g ammonium persulfate and boil 10 minutes; destroy excess persulfate by continued boiling.
  3. Buffer with sodium acetate to pH ~5; heat to 80 C.
  4. Add 10 mL 10% BaCl2 slowly with stirring; digest warm 30 minutes.
  5. Filter the yellow BaCrO4 through a weighed sintered-glass crucible.
  6. Wash with hot water; dry at 150 C to constant mass.
  7. Weigh BaCrO4; calculate % Cr.

Observations & Expected Results

Green Cr3+ solution turns orange-yellow on oxidation; bright yellow BaCrO4 precipitates, typically about 0.089 g from 1 g low-Cr steel.

Worked Stoichiometric Calculations

Problem: 1.000 g of steel gave 0.0885 g BaCrO4. Calculate % Cr. (GF_Cr = 0.2053)

Working: Mass Cr = 0.0885 × 0.2053 = 0.01817 g. % Cr = (0.01817/1.000) × 100 = 1.82%.

Safety Precautions & Hazard Control

  • Cr(VI) is carcinogenic: gloves and fume cupboard throughout.
  • Destroy excess persulfate fully or it oxidises Ba2+ side products.
  • Keep pH near 5; strongly acidic solution keeps chromate dissolved.

Waste Disposal Protocol

All Cr(VI) residues to dedicated chromium waste; reduce to Cr(III) before disposal per lab protocol.

Viva Voce Oral Defense Questions & Answers

Q: Why oxidise chromium to Cr(VI) first?

A: Cr3+ forms no stoichiometric barium precipitate; chromate gives the highly insoluble, stoichiometric BaCrO4.

Q: Why buffer to pH ~5?

A: In strong acid, chromate exists as dichromate/hydrogen chromate which precipitates incompletely; near pH 5 the CrO4 2- form dominates and BaCrO4 precipitates quantitatively.

← Back to Experiments Directory