CHEMVEN

Aluminium in Bauxite via 8-Hydroxyquinoline (Oxinate Method)

Determine aluminium in bauxite by precipitation as aluminium oxinate, Al(C9H6ON)3.

Level: UniversitySafety: Needs supervisionTime: 4 h
Aim of Experiment: Determine aluminium in bauxite by precipitation as aluminium oxinate, Al(C9H6ON)3.

Theoretical Foundations

8-Hydroxyquinoline (oxine) precipitates Al3+ quantitatively at pH 5-6: Al3+ + 3C9H7ON → Al(C9H6ON)3(s) + 3H+. The yellow chelate is stoichiometric and weighed directly after drying at 130 C — no ignition needed. The gravimetric factor is small (M_Al/M_complex = 26.98/459.43 = 0.05872), so a large precipitate mass gives excellent precision for small aluminium contents. Iron is masked or removed first.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 400 mL beaker
  • Hot plate
  • Sintered-glass crucible
  • Oven at 130 C
  • Desiccator
  • pH paper

Chemical Reagents

  • Bauxite sample, ground
  • Hydrochloric acid, dilute
  • 8-Hydroxyquinoline solution, 2% in ethanol
  • Ammonia solution, dilute
  • Ammonium acetate buffer
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.5 g bauxite; digest with 15 mL dilute HCl.
  2. Filter off insoluble residue; dilute the filtrate to 200 mL.
  3. Add ammonium acetate buffer; adjust to pH 5-6.
  4. Heat to 70 C; add 25 mL 2% oxine solution with stirring.
  5. Digest warm 30 minutes; filter the yellow precipitate through a weighed sintered-glass crucible.
  6. Wash with hot water; dry at 130 C to constant mass.
  7. Weigh Al(C9H6ON)3; calculate % Al and % Al2O3.

Observations & Expected Results

Yellow voluminous precipitate; typical mass about 0.89 g from 0.5 g bauxite.

Worked Stoichiometric Calculations

Problem: 0.5000 g of bauxite gave 0.8850 g Al(C9H6ON)3. Calculate % Al and % Al2O3. (GF_Al = 0.05872; Al in Al2O3 = 52.93%)

Working: Mass Al = 0.8850 × 0.05872 = 0.05197 g → % Al = 10.39%. % Al2O3 = (10.39/52.93) × 100 = 19.63%.

Safety Precautions & Hazard Control

  • Control pH at 5-6; outside this range precipitation is incomplete or Mg coprecipitates.
  • Remove iron first if high; Fe3+ also forms an oxinate.
  • Dry at 130 C; higher temperatures decompose the chelate.

Waste Disposal Protocol

Ethanolic oxine filtrates to organic waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is the gravimetric factor so small, and why is that good?

A: The bulky organic ligand makes the precipitate ~17 times heavier than the aluminium it contains, so weighing errors are divided by 17 — superb precision for small Al contents.

Q: Why buffer at pH 5-6?

A: Oxine precipitates Al quantitatively in this window; below pH 5 precipitation is incomplete, above pH 7 magnesium oxinate begins to coprecipitate.

← Back to Experiments Directory