CHEMVEN

Copper in Chalcopyrite Ore by Electrogravimetry

Determine copper in chalcopyrite ore after removing iron.

Level: UniversitySafety: Advanced lab onlyTime: 4 h
Aim of Experiment: Determine copper in chalcopyrite ore after removing iron.

Theoretical Foundations

Chalcopyrite (CuFeS2) is dissolved in HNO3; sulfur is oxidised to sulfate and iron removed as Fe(OH)3 with ammonia. Copper remains as the ammine, which is then acidified and electrolysed: Cu2+ + 2e- → Cu(s). The cathode gain gives % Cu directly; chalcopyrite concentrate is typically 25-35% Cu.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • Platinum cathode (weighed)
  • DC power supply
  • 400 mL beaker
  • Hot plate
  • Ashless filter paper
  • Oven
  • Desiccator

Chemical Reagents

  • Chalcopyrite ore, finely ground
  • Nitric acid, concentrated
  • Sulfuric acid, dilute
  • Ammonia solution, dilute
  • Distilled water
  • Ethanol

Step-by-Step Practical Procedure

  1. Weigh 0.6 g of ground ore; digest with 20 mL conc. HNO3 in a fume cupboard.
  2. Evaporate with 5 mL dilute H2SO4 to remove nitrate; dilute to 200 mL.
  3. Precipitate iron with dilute ammonia; filter off Fe(OH)3.
  4. Acidify the filtrate with H2SO4.
  5. Electrolyse at 2 A for 1 hour; test completeness.
  6. Wash with current on, dry and weigh the cathode; calculate % Cu.

Observations & Expected Results

Yellow sulfur oxidised away; brown Fe(OH)3 removed; blue filtrate yields a pink copper deposit, typically about 0.16 g.

Worked Stoichiometric Calculations

Problem: 0.6000 g of ore gave a cathode gain of 0.1580 g Cu. Calculate % Cu.

Working: % Cu = (0.1580/0.6000) × 100 = 26.33%.

Safety Precautions & Hazard Control

  • Remove iron fully or it codeposits/contaminates.
  • Fume off nitrate completely before electrolysis.
  • Grind the ore finely for complete attack.

Waste Disposal Protocol

Acidic iron/copper residues to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why remove iron before electrodepositing copper?

A: Fe3+ would be reduced at the cathode alongside copper (or oxidise the deposit), contaminating it and ruining the determination.

Q: What is the theoretical % Cu in pure chalcopyrite?

A: CuFeS2: 63.55/183.5 = 34.6% Cu; the ore at 26.3% is a lower-grade concentrate.