CHEMVEN

Lead as Lead Dioxide: Anodic Electrogravimetry

Determine lead in solder by anodic deposition as PbO2.

Level: UniversitySafety: Advanced lab onlyTime: 3 h
Aim of Experiment: Determine lead in solder by anodic deposition as PbO2.

Theoretical Foundations

Lead can be deposited on the anode as lead dioxide: Pb2+ + 2H2O → PbO2(s) + 4H+ + 2e-. The weighed PbO2 is converted to lead with the gravimetric factor M_Pb/M_PbO2 = 207.2/239.2 = 0.8662. Deposition is done in nitric acid at about 90 C with high current density; tin, if present, is removed first as metastannic acid.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • Platinum gauze anode (weighed)
  • DC power supply
  • 250 mL beaker
  • Hot plate
  • Fume cupboard
  • Oven
  • Desiccator

Chemical Reagents

  • Solder sample (Pb-Sn)
  • Nitric acid, concentrated and dilute
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh the Pt anode accurately.
  2. Weigh 0.5 g solder; dissolve in 15 mL conc. HNO3 in a fume cupboard.
  3. Evaporate to precipitate metastannic acid; filter it off.
  4. Dilute the filtrate to 150 mL with dilute HNO3; heat to 90 C.
  5. Electrolyse at 3-5 A for 45 minutes; brown PbO2 coats the anode.
  6. Wash the anode with the current on; dry at 180 C to constant mass.
  7. Weigh; calculate % Pb using GF = 0.8662.

Observations & Expected Results

Chocolate-brown adherent PbO2 on the anode; typical mass about 0.22 g from 0.5 g solder.

Worked Stoichiometric Calculations

Problem: 0.5000 g of solder gave 0.2150 g PbO2. Calculate % Pb. (GF_Pb = 0.8662)

Working: Mass Pb = 0.2150 × 0.8662 = 0.1862 g. % Pb = (0.1862/0.5000) × 100 = 37.25%.

Safety Precautions & Hazard Control

  • Remove tin first; it contaminates the anode deposit.
  • Dry PbO2 at 180 C; higher temperatures decompose it.
  • Keep the current on while washing the anode.

Waste Disposal Protocol

Acidic lead residues to heavy-metal waste; lead waste is toxic — collect all of it.

Viva Voce Oral Defense Questions & Answers

Q: Write the anode reaction for lead deposition.

A: Pb2+ + 2H2O → PbO2(s) + 4H+ + 2e-.

Q: Why dry PbO2 at 180 C and not higher?

A: Above ~200 C PbO2 begins to lose oxygen, giving non-stoichiometric oxides and low results.

Q: Why is this called anodic deposition?

A: The analyte deposits on the positive electrode (anode) by oxidation, the reverse of the usual cathodic metal deposition.