CHEMVEN

Copper in Electroplating Solution by Electrogravimetry

Determine the copper concentration (g/L) of an acid copper plating bath.

Level: UniversitySafety: SafeTime: 2 h
Aim of Experiment: Determine the copper concentration (g/L) of an acid copper plating bath.

Theoretical Foundations

Plating baths are assayed to maintain metal concentration. An aliquot is electrolysed directly: Cu2+ + 2e- → Cu(s). The cathode gain divided by the aliquot volume gives g/L Cu. Acid copper baths run typically 20-80 g/L Cu; the result guides replenishment additions.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 25 mL pipette
  • Analytical balance
  • Platinum electrodes
  • DC power supply
  • 250 mL beaker
  • Oven
  • Desiccator

Chemical Reagents

  • Acid copper plating bath sample
  • Sulfuric acid, dilute (if needed)
  • Distilled water
  • Ethanol

Step-by-Step Practical Procedure

  1. Pipette 25.00 mL of bath into a beaker; dilute to 150 mL if very concentrated.
  2. Weigh the Pt cathode.
  3. Electrolyse at 2 A with stirring for 45 minutes.
  4. Test completeness; wash with current on; rinse with ethanol and dry.
  5. Weigh the cathode; calculate g/L Cu.

Observations & Expected Results

Blue bath fades as copper deposits; typical gain about 1.9 g from 25 mL of bath.

Worked Stoichiometric Calculations

Problem: 25.00 mL of bath gave a cathode gain of 1.875 g Cu. Calculate the bath concentration in g/L.

Working: Concentration = 1.875 g / 0.02500 L = 75.0 g/L Cu.

Safety Precautions & Hazard Control

  • Pipette viscous bath samples carefully and rinse the pipette into the cell.
  • Ensure complete deposition; test on a fresh cathode surface.
  • Keep current on during washing.

Waste Disposal Protocol

Depleted bath sample to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why monitor plating bath copper concentration?

A: It controls the plating rate and deposit quality; depletion causes slow, poor plating, so the assay triggers replenishment.

Q: Why is this method well suited to plating baths?

A: The bath already contains only the analyte in a conductive acid medium — the sample can be electrolysed almost directly, with no separation needed.

← Back to Experiments Directory