Effect of Current Density on Copper Deposition

Show that excessive current density lowers current efficiency in copper electrogravimetry.

Level: UniversitySafety: Needs supervisionTime: 3 h
Aim of Experiment: Show that excessive current density lowers current efficiency in copper electrogravimetry.

Theoretical Foundations

Faraday's law gives the theoretical deposit: m = Q·M/(n·F). At moderate current density all current deposits copper (Cu2+ + 2e- → Cu). At very high current density the cathode potential shifts negative enough to evolve hydrogen as well (2H+ + 2e- → H2), wasting current: current efficiency = (actual/theoretical) × 100 falls, and the deposit turns dark and powdery.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • Platinum electrodes
  • DC power supply with ammeter
  • Two 250 mL beakers
  • Oven
  • Desiccator

Chemical Reagents

  • Copper sulfate standard solution (equal aliquots)
  • Sulfuric acid, dilute
  • Distilled water
  • Ethanol

Step-by-Step Practical Procedure

  1. Place identical aliquots of standard CuSO4 solution in two beakers; acidify equally.
  2. Weigh two cathodes.
  3. Electrolyse beaker A at 1 A (low current density) for 30 minutes.
  4. Electrolyse beaker B at 5 A (high current density) for the same charge-equivalent time adjusted to equal coulombs.
  5. Wash (current on), dry and weigh both deposits.
  6. Calculate current efficiency for each vs Faraday's law.

Observations & Expected Results

Deposit A is smooth and pink; deposit B is dark, rough and powdery, with visible gas bubbles during electrolysis.

Worked Stoichiometric Calculations

Problem: 2.00 A for 30.0 min should deposit 1.186 g Cu (Faraday's law). The high-current-density run gave 1.152 g. Calculate the current efficiency.

Working: Theoretical m = (3600 × 63.55)/(2 × 96485) = 1.186 g. Efficiency = (1.152/1.186) × 100 = 97.2% — the missing 2.8% of charge evolved hydrogen.

Safety Precautions & Hazard Control

  • Control the current, not just the voltage.
  • Vent hydrogen safely; no flames near the cell.
  • Compare equal total charge, not equal time, when currents differ.

Waste Disposal Protocol

Electrolytes to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: What is current efficiency?

A: The fraction of the total charge that produces the desired electrode reaction; side reactions like H2 evolution lower it below 100%.

Q: Why does the high-current-density deposit look dark and powdery?

A: Hydrogen bubbles disrupt crystal growth, giving a rough, burnt deposit that may also trap electrolyte.