CHEMVEN

Loss on Ignition of Limestone

Determine the loss on ignition (LOI) of limestone and relate it to carbonate content.

Level: UniversitySafety: Needs supervisionTime: 2 h
Aim of Experiment: Determine the loss on ignition (LOI) of limestone and relate it to carbonate content.

Theoretical Foundations

On ignition at 1000 C, carbonates decompose: CaCO3 → CaO + CO2↑. The mass loss (LOI) is essentially the CO2 content: % LOI = (loss/sample) × 100. For pure CaCO3 the theoretical LOI is 44.01/100.09 = 43.97%, so LOI/43.97 × 100 gives % CaCO3 — a rapid carbonate assay needing no reagents.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • Weighed porcelain crucible
  • Muffle furnace at 1000 C
  • Desiccator
  • Tongs

Chemical Reagents

  • Limestone sample, ground
  • Silica gel desiccant (for desiccator)
  • Distilled water (glassware rinsing)

Step-by-Step Practical Procedure

  1. Weigh a crucible (mass A); add about 1 g limestone; weigh (mass B).
  2. Ignite at 1000 C for 1 hour.
  3. Cool 30 minutes in a desiccator and weigh (mass C).
  4. Re-ignite 15 minutes to confirm constant mass.
  5. Calculate % LOI and hence % CaCO3.

Observations & Expected Results

Sample glows on ignition; no visible change otherwise; typical loss about 0.44 g from 1 g limestone.

Worked Stoichiometric Calculations

Problem: Crucible 25.0000 g; crucible + limestone 26.0000 g; after ignition 25.5620 g. Calculate % LOI and % CaCO3.

Working: Loss = 26.0000 − 25.5620 = 0.4380 g. % LOI = 43.80%. % CaCO3 = (43.80/43.97) × 100 = 99.6%.

Safety Precautions & Hazard Control

  • Ignite long enough to decompose all carbonate.
  • Cool in a desiccator; CaO residue reabsorbs CO2 and water.
  • Use a representative ground sample.

Waste Disposal Protocol

Ignited residue to solid waste.

Viva Voce Oral Defense Questions & Answers

Q: What does LOI measure in a limestone?

A: Essentially the CO2 driven off from carbonates (plus any organic matter and combined water), so it quantifies the carbonate content.

Q: Why is LOI a standard test in cement works?

A: It is a fast, reagent-free check of limestone purity for raw-mix control, run routinely alongside full oxide analysis.

← Back to Experiments Directory