CHEMVEN

Ash in Paper: Filler and Coating Analysis

Determine the ash (mineral filler) content of printing paper.

Level: UniversitySafety: Needs supervisionTime: 3 h
Aim of Experiment: Determine the ash (mineral filler) content of printing paper.

Theoretical Foundations

Paper contains mineral fillers (clay, calcium carbonate, TiO2) that improve opacity and printability. Ignition at 525 C burns the cellulose: % ash = (residue/sample) × 100. The modest temperature avoids decomposing CaCO3 filler, so the ash approximates the true filler loading.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • Weighed crucible
  • Muffle furnace at 525 C
  • Desiccator
  • Tongs

Chemical Reagents

  • Paper sample, cut in strips
  • Silica gel desiccant (for desiccator)
  • Distilled water (glassware rinsing)

Step-by-Step Practical Procedure

  1. Weigh a crucible (mass A); add about 2 g of paper strips; weigh (mass B).
  2. Ignite gently at first to char the paper without flaming.
  3. Ash at 525 C for 2 hours to a white residue.
  4. Cool in a desiccator and weigh (mass C).
  5. Re-ignite to constant mass; calculate % ash.

Observations & Expected Results

Paper chars then burns to a white powdery ash, typically about 0.014 g from 2 g paper.

Worked Stoichiometric Calculations

Problem: Crucible 20.0000 g; crucible + paper 22.0000 g; crucible + ash 20.0140 g. Calculate % ash.

Working: % ash = (0.0140/2.0000) × 100 = 0.70% — a low filler loading, typical of an uncoated sheet.

Safety Precautions & Hazard Control

  • Char slowly; paper flares easily and can eject ash.
  • 525 C preserves CaCO3 filler; higher temperatures decompose it.
  • Cool in a desiccator; the ash is hygroscopic.

Waste Disposal Protocol

Paper ash to general waste.

Viva Voce Oral Defense Questions & Answers

Q: Why ash paper at only 525 C?

A: To burn cellulose completely while leaving calcium carbonate filler undecomposed, so the ash mass reflects the true mineral loading.

Q: What fillers are used in paper and why?

A: Clay, calcium carbonate and titanium dioxide — they fill fibre gaps, raising opacity, brightness and smoothness for printing.

← Back to Experiments Directory