Moisture in Coal: Air-Drying Loss
Determine the surface (air-drying) moisture of coal.
Theoretical Foundations
Coal moisture is split into surface moisture (lost by air-drying) and inherent moisture. The air-drying loss at ~40 C with ventilation gives surface moisture: % = (loss/sample) × 100. Moisture lowers the calorific value per kilogram as received and affects handling and pricing of coal.
Required Apparatus & Chemicals
Laboratory Apparatus
- Analytical balance
- Weighed tray or dish
- Air oven at 40 C with ventilation
- Desiccator
Chemical Reagents
- Coal sample, air-dried lab sample
- Silica gel desiccant (for desiccator)
- Distilled water (glassware rinsing)
Step-by-Step Practical Procedure
- Weigh a tray (mass A); spread about 10 g of coal in a thin layer.
- Weigh tray + coal (mass B).
- Dry in a ventilated oven at 40 C for 2 hours.
- Cool in a desiccator and weigh (mass C).
- Repeat drying to constant mass.
- Calculate % air-drying moisture.
Observations & Expected Results
Coal darkens slightly as surface water evaporates; typical loss about 0.28 g from 10 g coal.
Worked Stoichiometric Calculations
Problem: Tray 50.000 g; tray + coal 60.000 g; after drying 59.720 g. Calculate % surface moisture.
Working: Loss = 60.000 − 59.720 = 0.280 g from 10.000 g. % moisture = (0.280/10.000) × 100 = 2.80%.
Safety Precautions & Hazard Control
- Use gentle 40 C drying; higher temperatures oxidise coal and drive off inherent moisture too.
- Spread thinly for even drying.
- Weigh promptly after cooling.
Waste Disposal Protocol
Dried coal to solid fuel waste.
Viva Voce Oral Defense Questions & Answers
Q: What is the difference between surface and inherent moisture?
A: Surface moisture is free water on particle surfaces, lost by air-drying; inherent (bed) moisture is held in pores and needs 105 C to remove.
Q: Why does moisture matter in coal trading?
A: Coal is sold by mass but valued by energy; moisture adds dead weight and consumes heat on evaporation, lowering the useful calorific value.