Double Dehydration of Silicic Acid: Recovery Study
Quantify how much silica is recovered by the second dehydration in cement analysis.
Theoretical Foundations
A single evaporation leaves some silicic acid as a colloid that passes through the filter. Re-evaporating the filtrate dehydrates this residual silica: H2SiO3 → SiO2 + H2O. Each fraction is ignited, weighed and HF-corrected separately, showing that the second dehydration typically recovers 1-3% of the total silica — small but significant for accurate cement analysis.
Required Apparatus & Chemicals
Laboratory Apparatus
- Analytical balance
- 250 mL beakers
- Hot plate
- Oven and muffle furnace
- Ashless filter paper
- Platinum crucible
- Desiccator
- HF handling kit
Chemical Reagents
- Portland cement sample
- Hydrochloric acid, concentrated
- Hydrofluoric acid
- Sulfuric acid, dilute
- Distilled water
Step-by-Step Practical Procedure
- Weigh accurately 1.0 g cement; decompose with conc. HCl.
- Evaporate to dryness; bake 1 hour at 110 C (first dehydration).
- Take up with HCl, filter; ignite the residue and HF-correct it (silica fraction 1).
- Evaporate the filtrate to dryness again; bake and filter (second dehydration).
- Ignite and HF-correct fraction 2.
- Calculate each fraction's % SiO2 and the total.
Observations & Expected Results
First fraction is the bulk of the silica; the second is a small but visible residue.
Worked Stoichiometric Calculations
Problem: 1.000 g cement: fraction 1 gave 0.2060 g HF-volatile SiO2; fraction 2 gave 0.0075 g. Calculate total % SiO2 and the % recovered by the second dehydration.
Working: Total SiO2 = 0.2060 + 0.0075 = 0.2135 g → 21.35%. Second dehydration recovered (0.0075/0.2135) × 100 = 3.5% of the silica — omitted at the cost of a 0.75% absolute error.
Safety Precautions & Hazard Control
- Bake both dehydrations fully.
- HF safety measures as before.
- Keep the two fractions separate until weighed.
Waste Disposal Protocol
Fluoride waste to dedicated containers.
Viva Voce Oral Defense Questions & Answers
Q: Why does some silica escape the first dehydration?
A: Part of the silicic acid remains as a stable colloid that is not fully dehydrated in one evaporation and passes through the filter paper.
Q: Is double dehydration always necessary?
A: For referee cement analysis yes; for rapid control work a single dehydration with an empirical correction is sometimes accepted.