CHEMVEN

Silica in Rice Husk Ash: Agricultural Waste Valorisation

Determine silica in rice husk ash to assess it as a pozzolan/silica source.

Level: UniversitySafety: Needs supervisionTime: 4 h
Aim of Experiment: Determine silica in rice husk ash to assess it as a pozzolan/silica source.

Theoretical Foundations

Rice husk ash is 85-95% amorphous silica. Acid leaching removes alkali and iron impurities; the residue is ignited and weighed, then HF-volatilised: SiO2 + 4HF → SiF4↑ + 2H2O. The high silica content makes the ash valuable as a cement pozzolan and silica feedstock.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 250 mL beaker
  • Hot plate
  • Ashless filter paper
  • Platinum crucible
  • Muffle furnace
  • Desiccator
  • HF handling kit

Chemical Reagents

  • Rice husk ash sample
  • Hydrochloric acid, dilute
  • Hydrofluoric acid
  • Sulfuric acid, dilute
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.5 g of rice husk ash.
  2. Digest with 20 mL dilute HCl for 20 minutes to leach impurities.
  3. Filter through ashless paper; wash the residue.
  4. Ignite at 1000 C to constant mass; weigh (mass A).
  5. Treat with HF + H2SO4 in a fume cupboard; evaporate and reignite; weigh (mass B).
  6. Calculate % SiO2 = (A − B)/sample × 100.

Observations & Expected Results

Grey ash lightens on acid leaching; white residue; large mass loss on HF treatment.

Worked Stoichiometric Calculations

Problem: 0.5000 g of ash: mass A = 0.4780 g, mass B = 0.0160 g. Calculate % SiO2.

Working: SiO2 = 0.4780 − 0.0160 = 0.4620 g. % SiO2 = (0.4620/0.5000) × 100 = 92.4% — excellent pozzolanic material.

Safety Precautions & Hazard Control

  • HF safety: full PPE, fume cupboard, calcium gluconate gel available.
  • Leach fully; residual alkali inflates the non-volatile residue.
  • Ignite to constant mass; ash adsorbs moisture.

Waste Disposal Protocol

Fluoride waste to dedicated containers.

Viva Voce Oral Defense Questions & Answers

Q: What is a pozzolan?

A: A siliceous material that reacts with calcium hydroxide in the presence of water to form cementitious compounds, improving concrete strength and durability.

Q: Why is rice husk ash silica amorphous rather than quartz?

A: It forms at relatively low combustion temperatures from biogenic silica in the husk, giving a reactive amorphous form rather than crystalline quartz.