CHEMVEN

Silica in Soda-Lime Glass

Determine SiO2 in soda-lime glass by carbonate fusion and dehydration.

Level: UniversitySafety: Advanced lab onlyTime: 4 h
Aim of Experiment: Determine SiO2 in soda-lime glass by carbonate fusion and dehydration.

Theoretical Foundations

Glass resists acid attack, so it is fused with sodium carbonate: Na2CO3 + SiO2 → Na2SiO3 + CO2. Dissolving the melt in HCl gives silicic acid, which is dehydrated by double evaporation: H2SiO3 → SiO2 + H2O. The ignited silica is weighed, with HF volatilisation correcting for impurities. Soda-lime glass is ~72% SiO2.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • Platinum crucible
  • Muffle furnace
  • 250 mL beaker
  • Hot plate
  • Ashless filter paper
  • Desiccator
  • HF handling kit

Chemical Reagents

  • Glass sample, finely ground
  • Sodium carbonate, anhydrous
  • Hydrochloric acid, concentrated
  • Hydrofluoric acid
  • Sulfuric acid, dilute
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 1.0 g of finely ground glass.
  2. Mix with 5 g anhydrous Na2CO3 in a platinum crucible; fuse at 1000 C for 30 minutes.
  3. Dissolve the cold melt in dilute HCl in a beaker.
  4. Evaporate to dryness; bake 1 hour at 110 C.
  5. Take up with HCl, filter the silica; repeat dehydration on the filtrate.
  6. Ignite combined silica at 1000 C to constant mass; weigh.
  7. Correct with HF volatilisation; the mass loss is true SiO2.
  8. Calculate % SiO2.

Observations & Expected Results

Clear fusion melt; gelatinous silica; white ignited SiO2, typically about 0.72 g from 1 g glass.

Worked Stoichiometric Calculations

Problem: 1.000 g of glass gave 0.7150 g of HF-volatile SiO2. Calculate % SiO2.

Working: % SiO2 = (0.7150/1.000) × 100 = 71.5%, the normal soda-lime glass composition.

Safety Precautions & Hazard Control

  • Grind glass very finely or fusion is incomplete.
  • HF: full PPE and fume cupboard mandatory.
  • Cool the melt before adding acid to avoid violent spattering.

Waste Disposal Protocol

Fluoride waste to dedicated containers; fusion residues neutralised.

Viva Voce Oral Defense Questions & Answers

Q: Why fuse glass instead of acid-digesting it?

A: The silicate network of glass is inert to acids (except HF); carbonate fusion converts it to soluble alkali silicate.

Q: What are the other major oxides in soda-lime glass?

A: Na2O (~13%) and CaO (~10%), which lower the melting point and working temperature compared with pure silica glass.

← Back to Experiments Directory