Silica in Sand: High-Purity Material Assay

Determine the SiO2 content of a foundry sand by acid digestion and HF volatilisation.

Level: UniversitySafety: Needs supervisionTime: 4 h
Aim of Experiment: Determine the SiO2 content of a foundry sand by acid digestion and HF volatilisation.

Theoretical Foundations

Sand is mostly quartz (SiO2) with clay and iron oxide impurities. Digestion in HCl dissolves carbonates and iron oxides; the residue is ignited and weighed, then treated with HF: SiO2 + 4HF → SiF4↑ + 2H2O. The mass lost on HF treatment is the true silica; the non-volatile residue is impurity. % SiO2 = (loss/sample mass) × 100.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 250 mL beaker
  • Hot plate
  • Ashless filter paper
  • Platinum crucible
  • Muffle furnace
  • Desiccator
  • HF handling kit

Chemical Reagents

  • Sand sample, dried
  • Hydrochloric acid, dilute
  • Hydrofluoric acid
  • Sulfuric acid, dilute
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.5 g of dried sand.
  2. Digest with 20 mL dilute HCl on a hot plate for 20 minutes.
  3. Filter through ashless paper; wash the residue.
  4. Transfer to a platinum crucible; ignite at 1000 C to constant mass and weigh (mass A).
  5. In a fume cupboard add HF and a few drops of H2SO4; evaporate to dryness.
  6. Reignite at 1000 C; weigh (mass B).
  7. SiO2 = A − B; calculate % SiO2.

Observations & Expected Results

Sand largely undissolved by HCl; white residue; mass drops sharply after HF treatment.

Worked Stoichiometric Calculations

Problem: 0.5000 g of sand: mass A = 0.4960 g, mass B = 0.0135 g. Calculate % SiO2.

Working: SiO2 = 0.4960 − 0.0135 = 0.4825 g. % SiO2 = (0.4825/0.5000) × 100 = 96.5%.

Safety Precautions & Hazard Control

  • HF causes deep tissue burns: full PPE, fume cupboard, calcium gluconate gel on hand.
  • Never store or heat HF in glass; use platinum or PTFE.
  • Drive off all fluoride with H2SO4 before the final ignition.

Waste Disposal Protocol

All fluoride waste to dedicated HF waste containers.

Viva Voce Oral Defense Questions & Answers

Q: Write the reaction of silica with HF.

A: SiO2 + 4HF → SiF4↑ + 2H2O; silicon tetrafluoride is volatile.

Q: Why add sulfuric acid with the HF?

A: To convert fluorides of impurities to non-volatile sulfates and ensure complete expulsion of silicon as SiF4.

Q: What limits foundry sand quality?

A: Clay content and grain-size distribution, which control the sand's bonding and permeability in moulding.