CHEMVEN

Magnesium in Magnalium Alloy

Determine magnesium in a magnalium (Al-Mg) alloy after removing aluminium.

Level: UniversitySafety: Needs supervisionTime: 4 h
Aim of Experiment: Determine magnesium in a magnalium (Al-Mg) alloy after removing aluminium.

Theoretical Foundations

The alloy is dissolved in HCl; aluminium is precipitated with ammonia as Al(OH)3 and filtered off (magnesium stays soluble). Magnesium is then precipitated: Mg2+ + NH4+ + HPO4 2- → MgNH4PO4(s) + H+, ignited to Mg2P2O7 (GF = 0.2184). Magnalium typically contains 5-30% Mg.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 400 mL beaker
  • Hot plate
  • Ashless filter paper
  • Porcelain crucible
  • Muffle furnace
  • Desiccator

Chemical Reagents

  • Magnalium alloy sample
  • Hydrochloric acid, dilute
  • Ammonia solution, dilute and concentrated
  • Diammonium hydrogen phosphate solution, 10%
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.4 g of alloy; dissolve in 15 mL dilute HCl with warming.
  2. Dilute to 200 mL; add dilute ammonia to precipitate Al(OH)3 (just alkaline); filter off.
  3. Acidify the filtrate slightly; add 15 mL 10% (NH4)2HPO4.
  4. Add concentrated ammonia with stirring to strong alkalinity plus excess; stand 4 hours.
  5. Filter, wash with dilute ammonia, ignite at 1000 C to constant mass.
  6. Weigh Mg2P2O7; calculate % Mg.

Observations & Expected Results

Gelatinous Al(OH)3 filtered off; white crystalline magnesium precipitate; white Mg2P2O7, typically about 0.165 g from 0.4 g alloy.

Worked Stoichiometric Calculations

Problem: 0.4000 g of magnalium gave 0.1650 g Mg2P2O7. Calculate % Mg.

Working: Mass Mg = 0.1650 × 0.2184 = 0.03604 g. % Mg = (0.03604/0.4000) × 100 = 9.01%.

Safety Precautions & Hazard Control

  • Remove aluminium quantitatively or it contaminates the phosphate precipitate.
  • Do not precipitate Al(OH)3 with a large excess of ammonia (it redissolves).
  • Stand the magnesium precipitate long enough.

Waste Disposal Protocol

Acidic/alkaline metal filtrates neutralised; residues to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is aluminium removed before precipitating magnesium?

A: Al3+ would precipitate as AlPO4 with the phosphate reagent, contaminating the MgNH4PO4 and giving high results.

Q: Why does Al(OH)3 redissolve in excess ammonia only slightly, unlike with NaOH?

A: Al(OH)3 is amphoteric toward strong base (forming aluminate) but only very slightly soluble in ammonia, so a small excess of ammonia is safe.

← Back to Experiments Directory