Calcium in Portland Cement (CaO by Oxalate Ignition)

Determine CaO in Portland cement after removing silica, iron and aluminium.

Level: UniversitySafety: Needs supervisionTime: 4 h
Aim of Experiment: Determine CaO in Portland cement after removing silica, iron and aluminium.

Theoretical Foundations

Cement analysis is sequential: silica is dehydrated and filtered off, then Fe(OH)3 and Al(OH)3 are precipitated with ammonia (the R2O3 group) and filtered off. Calcium remains and is precipitated as oxalate: Ca2+ + C2O4 2- → CaC2O4(s), ignited at 1000 C to CaO (GF for Ca = 0.7147; results reported as % CaO directly from the ignited mass). Typical Portland cement is ~65% CaO.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 250 mL beakers
  • Hot plate
  • Quantitative and ashless filter papers
  • Porcelain crucible
  • Muffle furnace
  • Desiccator

Chemical Reagents

  • Portland cement sample
  • Hydrochloric acid, concentrated and dilute
  • Ammonia solution, dilute
  • Ammonium oxalate solution, 4%
  • Methyl red indicator
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.5 g cement; decompose with HCl, dehydrate silica and filter it off.
  2. To the filtrate add ammonia to precipitate R2O3 (Fe, Al); filter off.
  3. Dilute the filtrate to 200 mL; add methyl red and heat.
  4. Precipitate calcium with hot ammonium oxalate; adjust to yellow endpoint.
  5. Digest, filter through ashless paper, wash with cold water.
  6. Ignite at 1000 C to constant mass; cool and weigh CaO quickly.
  7. Calculate % CaO = (mass CaO / sample mass) × 100.

Observations & Expected Results

Sequential precipitates: gelatinous silica, brown R2O3, then white calcium oxalate; final white CaO, typically about 0.33 g from 0.5 g cement.

Worked Stoichiometric Calculations

Problem: 0.5000 g of cement gave 0.3250 g CaO. Calculate % CaO and % Ca. (GF_Ca = 0.7147)

Working: % CaO = (0.3250/0.5000) × 100 = 65.0%. Mass Ca = 0.3250 × 0.7147 = 0.2323 g → % Ca = 46.46%.

Safety Precautions & Hazard Control

  • Remove silica and R2O3 quantitatively first; they contaminate the oxalate.
  • Ignite at 1000 C to decompose CaCO3 fully.
  • Weigh CaO fast; it picks up moisture and CO2.

Waste Disposal Protocol

Acidic filtrates neutralised.

Viva Voce Oral Defense Questions & Answers

Q: Outline the classical cement analysis sequence.

A: Acid decomposition → silica by dehydration → R2O3 (Fe2O3 + Al2O3) by ammonia precipitation → CaO by oxalate precipitation and ignition → MgO by difference or as pyrophosphate.

Q: Why is calcium determined after iron and aluminium?

A: Fe3+ and Al3+ would coprecipitate with calcium oxalate; removing them as hydroxides first gives a clean calcium separation.