Iron in Rust: Composition of Corrosion Product
Determine the iron content of rust to characterise the corrosion product.
Theoretical Foundations
Rust is hydrated ferric oxide, approximately Fe2O3·xH2O, often contaminated with salts. Dissolving in HCl gives Fe3+ in solution; precipitation with ammonia and ignition drives off all water: 2Fe(OH)3 → Fe2O3 + 3H2O (GF = 0.6994). The % Fe found, compared with 69.94% for pure Fe2O3, indicates the degree of hydration and contamination.
Required Apparatus & Chemicals
Laboratory Apparatus
- Analytical balance
- 250 mL beaker
- Hot plate
- Ashless filter paper
- Porcelain crucible
- Muffle furnace
- Desiccator
Chemical Reagents
- Rust sample, ground
- Hydrochloric acid, dilute
- Nitric acid, concentrated
- Ammonia solution, dilute
- Ammonium chloride, solid
- Distilled water
Step-by-Step Practical Procedure
- Weigh accurately 0.5 g of ground rust.
- Dissolve in 15 mL dilute HCl with warming; add a drop of conc. HNO3.
- Dilute to 150 mL; filter off any insoluble residue.
- Add NH4Cl, precipitate Fe(OH)3 with dilute ammonia.
- Filter, wash chloride-free, ignite at 850 C to constant mass.
- Weigh Fe2O3 and calculate % Fe in the rust.
Observations & Expected Results
Rust dissolves to a yellow-brown solution; brown precipitate ignites to reddish Fe2O3, typically about 0.39 g.
Worked Stoichiometric Calculations
Problem: 0.5000 g of rust gave 0.3850 g Fe2O3. Calculate % Fe and comment.
Working: Mass Fe = 0.3850 × 0.6994 = 0.2693 g. % Fe = (0.2693/0.5000) × 100 = 53.85%. Well below 69.94% for Fe2O3, confirming rust is heavily hydrated and contains non-ferrous contaminants.
Safety Precautions & Hazard Control
- Grind rust finely for complete dissolution.
- Remove any paint or metallic iron flakes before weighing.
- Ignite to constant mass to expel all water.
Waste Disposal Protocol
Acidic filtrates neutralised.
Viva Voce Oral Defense Questions & Answers
Q: What is the approximate formula of rust?
A: Hydrated ferric oxide, Fe2O3·xH2O (often written FeOOH·nH2O), with x variable — which is why % Fe is below 69.94%.
Q: Why can't rust be weighed directly as the analytical form?
A: Its water content is variable and non-stoichiometric; ignition converts it to the definite compound Fe2O3.