CHEMVEN

Iron in Steel Wire: High-Purity Matrix

Determine iron in mild-steel wire (≈99% Fe) by hydroxide gravimetry.

Level: UniversitySafety: Needs supervisionTime: 3 h
Aim of Experiment: Determine iron in mild-steel wire (≈99% Fe) by hydroxide gravimetry.

Theoretical Foundations

Steel wire dissolves in HCl/HNO3; alloying elements (Mn, Si) are at low levels and mostly stay in solution or are filtered as silica. Fe3+ is precipitated with ammonia: Fe3+ + 3OH- → Fe(OH)3(s), then ignited to Fe2O3 (GF = 0.6994). For a ~99% Fe matrix the method tests precision: small absolute errors are visible as deviations from 100%.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 400 mL beaker
  • Hot plate
  • Ashless filter paper
  • Porcelain crucible
  • Muffle furnace
  • Desiccator

Chemical Reagents

  • Steel wire pieces
  • Hydrochloric acid, dilute
  • Nitric acid, concentrated
  • Ammonia solution, dilute
  • Ammonium chloride, solid
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.4 g of clean steel wire pieces.
  2. Dissolve in 15 mL dilute HCl with 2 mL conc. HNO3 on a hot plate.
  3. Dilute to 200 mL; filter off any silica residue.
  4. Add NH4Cl, heat to boiling, precipitate with dilute ammonia.
  5. Digest, filter, wash with hot 1% NH4Cl until chloride-free.
  6. Ignite at 850 C to constant mass; weigh Fe2O3 and calculate % Fe.

Observations & Expected Results

Wire dissolves with effervescence; brown precipitate ignites to reddish Fe2O3, typically about 0.57 g from 0.4 g wire.

Worked Stoichiometric Calculations

Problem: 0.4000 g of steel wire gave 0.5680 g Fe2O3. Calculate % Fe.

Working: Mass Fe = 0.5680 × 0.6994 = 0.3973 g. % Fe = (0.3973/0.4000) × 100 = 99.31%, as expected for mild steel.

Safety Precautions & Hazard Control

  • Clean the wire of oil/rust before weighing.
  • Oxidise fully to Fe3+.
  • Avoid a large excess of ammonia, which makes the precipitate slimy.

Waste Disposal Protocol

Acidic filtrates neutralised; iron residues to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is this determination a good precision test?

A: Because the true value is near 100%, any procedural error shows up directly as a deviation from 100% without being masked by matrix corrections.

Q: What happens to manganese in this procedure?

A: Mn2+ partly precipitates as Mn(OH)2 and oxidises on ignition to Mn3O4, causing a small positive error; it is negligible in mild steel.

← Back to Experiments Directory