CHEMVEN

Iron in Hematite Ore: Hydroxide Precipitation, Ignition to Fe2O3

Determine iron in hematite ore by precipitating Fe(OH)3 and igniting to Fe2O3.

Level: UniversitySafety: Needs supervisionTime: 3 h
Aim of Experiment: Determine iron in hematite ore by precipitating Fe(OH)3 and igniting to Fe2O3.

Theoretical Foundations

The ore is dissolved in HCl; Fe2+ is oxidised to Fe3+ with HNO3. Adding ammonia precipitates gelatinous brown Fe(OH)3: Fe3+ + 3OH- → Fe(OH)3(s). The hydroxide is non-stoichiometric, so it is ignited: 2Fe(OH)3 → Fe2O3 + 3H2O. Ferric oxide is stable and stoichiometric; the gravimetric factor for iron is 2 × M_Fe/M_Fe2O3 = 111.69/159.69 = 0.6994.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 400 mL beaker
  • Hot plate
  • Ashless filter paper
  • Porcelain crucible
  • Muffle furnace
  • Desiccator

Chemical Reagents

  • Hematite ore, finely ground
  • Hydrochloric acid, concentrated and dilute
  • Nitric acid, concentrated
  • Ammonia solution, dilute (1+1)
  • Ammonium chloride, solid
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.4-0.5 g of ground ore.
  2. Dissolve in 15 mL conc. HCl with warming; add 2 mL conc. HNO3 to oxidise Fe2+ to Fe3+.
  3. Evaporate to low volume, dilute to 200 mL and filter off insoluble silica.
  4. Add 2 g NH4Cl, heat to boiling and add dilute ammonia with stirring until just alkaline plus slight excess.
  5. Digest warm 15 minutes; filter the brown precipitate through ashless paper.
  6. Wash with hot 1% NH4Cl solution until chloride-free.
  7. Transfer to a crucible, char the paper, ignite at 800-900 C to constant mass, cool and weigh Fe2O3.

Observations & Expected Results

Brown gelatinous precipitate; on ignition it becomes reddish-brown Fe2O3. Typical mass about 0.44 g from 0.5 g ore.

Worked Stoichiometric Calculations

Problem: 0.5000 g of hematite gave 0.4432 g Fe2O3. Calculate % Fe. (GF_Fe = 0.6994)

Working: Mass Fe = 0.4432 × 0.6994 = 0.3100 g. % Fe = (0.3100/0.5000) × 100 = 62.0%. (Pure Fe2O3 is 69.94% Fe, so the ore is 88.6% Fe2O3.)

Safety Precautions & Hazard Control

  • Oxidise all Fe2+ to Fe3+; Fe(OH)2 oxidises unpredictably on ignition.
  • Add NH4Cl before ammonia to give a more filterable precipitate.
  • Wash with NH4Cl solution, not pure water, to prevent peptization.

Waste Disposal Protocol

Acidic iron filtrates are neutralised; iron residues to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is Fe2+ oxidised to Fe3+ before precipitation?

A: Fe(OH)2 is gelatinous, oxidises in air to non-stoichiometric products and gives erratic ignition masses; Fe(OH)3 ignites cleanly to stoichiometric Fe2O3.

Q: Why wash Fe(OH)3 with NH4Cl solution?

A: Pure water peptizes the gelatinous hydroxide, sending colloidal iron through the filter; volatile NH4Cl keeps it coagulated and leaves no residue on ignition.

Q: Why ignite at 800-900 C?

A: To decompose Fe(OH)3 fully to Fe2O3 and burn the paper; below ~700 C conversion is incomplete, above ~1000 C Fe2O3 can reduce slightly.

← Back to Experiments Directory