Nickel in Spent Hydrogenation Catalyst

Determine nickel in a spent supported catalyst (Ni on alumina/silica) for metal-recovery assessment.

Level: UniversitySafety: Needs supervisionTime: 3 h
Aim of Experiment: Determine nickel in a spent supported catalyst (Ni on alumina/silica) for metal-recovery assessment.

Theoretical Foundations

Spent catalysts are leached with acid to dissolve nickel, leaving the silica/alumina support largely undissolved: NiO + 2H+ → Ni2+ + H2O. After filtering off the support, nickel is precipitated: Ni2+ + 2 H2DMG → Ni(HDMG)2(s) + 2H+, GF = 0.2032. The result decides whether metal recovery is economic.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 250 mL beaker
  • Hot plate
  • Quantitative filter paper
  • Sintered-glass crucible
  • Oven
  • Desiccator

Chemical Reagents

  • Spent catalyst, ground
  • Hydrochloric acid, dilute (1+1)
  • Dimethylglyoxime solution, 1% in ethanol
  • Ammonia solution, dilute
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.6 g of ground spent catalyst.
  2. Digest with 25 mL dilute HCl on a hot plate for 30 minutes with stirring.
  3. Filter off the undissolved support through quantitative paper; wash well.
  4. Dilute the filtrate to 150 mL; add DMG at 70-80 C, then ammonia to pH 8-9.
  5. Digest, filter through a weighed sintered-glass crucible, wash and dry at 150 C.
  6. Weigh Ni(DMG)2 to constant mass and calculate % Ni.

Observations & Expected Results

Dark catalyst powder leaves a pale support residue; greenish filtrate gives a scarlet precipitate, typically about 0.3 g.

Worked Stoichiometric Calculations

Problem: 0.6000 g of spent catalyst gave 0.2950 g Ni(DMG)2. Calculate % Ni.

Working: Mass Ni = 0.2950 × 0.2032 = 0.05994 g. % Ni = (0.05994/0.6000) × 100 = 9.99% ≈ 10.0% Ni — worth recovering.

Safety Precautions & Hazard Control

  • Leach long enough to dissolve all accessible nickel.
  • Wash the support residue thoroughly; occluded nickel solution causes low results.
  • Some catalysts are pyrophoric when dry; keep the sample damp until leached.

Waste Disposal Protocol

Acidic nickel leachates to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why filter off the support before precipitating nickel?

A: Silica/alumina fines would contaminate the Ni(DMG)2 precipitate and adsorb nickel ions, giving erratic results.

Q: What nickel level makes recovery economic?

A: It depends on metal prices, but spent catalysts above roughly 5-10% Ni are commonly sent for metal recovery rather than landfill.