Nickel in Laterite Ore as Ni(DMG)2

Determine low-grade nickel in a laterite ore by DMG gravimetry after iron removal.

Level: UniversitySafety: Needs supervisionTime: 4 h
Aim of Experiment: Determine low-grade nickel in a laterite ore by DMG gravimetry after iron removal.

Theoretical Foundations

Laterites contain 1-3% Ni in a matrix of iron oxides. The ore is dissolved in acid; iron is removed by precipitating Fe(OH)3 with ammonia (nickel stays soluble as the ammine at controlled pH, or is separated by double precipitation). Nickel is then precipitated: Ni2+ + 2 H2DMG → Ni(HDMG)2(s) + 2H+, GF = 0.2032. A 1 g sample keeps the precipitate weighable despite the low grade.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 250 mL beakers
  • Hot plate
  • Quantitative filter paper
  • Sintered-glass crucible
  • Oven
  • Desiccator

Chemical Reagents

  • Laterite ore, finely ground
  • Hydrochloric acid, concentrated and dilute
  • Ammonia solution
  • Dimethylglyoxime solution, 1% in ethanol
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 1.0 g of ground ore.
  2. Digest with 20 mL conc. HCl on a hot plate until decomposed; evaporate to low volume.
  3. Dilute to 150 mL, add ammonia to precipitate Fe(OH)3 at pH ~4 (methyl red endpoint); filter off iron.
  4. To the filtrate add DMG solution at 70-80 C, then ammonia to pH 8-9.
  5. Digest, filter the scarlet precipitate through a weighed sintered-glass crucible.
  6. Wash, dry at 150 C to constant mass and weigh; calculate % Ni.

Observations & Expected Results

Bulky brown Fe(OH)3 is filtered off; the pale filtrate gives a small scarlet precipitate, typically 0.05-0.10 g.

Worked Stoichiometric Calculations

Problem: 1.000 g of laterite gave 0.0725 g Ni(DMG)2. Calculate % Ni in the ore.

Working: Mass Ni = 0.0725 × 0.2032 = 0.01473 g. % Ni = (0.01473/1.000) × 100 = 1.47%.

Safety Precautions & Hazard Control

  • Remove iron quantitatively or it contaminates the nickel precipitate.
  • Grind the ore finely for complete acid attack.
  • Work in a fume cupboard during acid digestion.

Waste Disposal Protocol

Acidic iron/nickel residues to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is iron removed before the nickel precipitation?

A: Fe3+ would precipitate as Fe(OH)3 when ammonia is added for the DMG step, massively contaminating the small nickel precipitate.

Q: Why take a full 1 g sample?

A: At 1-2% Ni the precipitate from a smaller sample would be too light to weigh accurately; a larger sample gives a weighable mass.