CHEMVEN

Chloride in Cement: Corrosion-Risk Assessment

Determine acid-soluble chloride in cement to assess the risk of steel-reinforcement corrosion.

Level: UniversitySafety: Needs supervisionTime: 3 h
Aim of Experiment: Determine acid-soluble chloride in cement to assess the risk of steel-reinforcement corrosion.

Theoretical Foundations

Chloride above about 0.4% by mass of cement depassivates steel reinforcement and initiates corrosion. Cement is digested in nitric acid (not HCl, which would add chloride), silica is filtered off, and chloride is precipitated: Ag+ + Cl- → AgCl(s). GF = 0.2473 gives % Cl for comparison with the corrosion threshold.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 250 mL beaker
  • Hot plate
  • Quantitative filter paper
  • Sintered-glass crucible
  • Oven
  • Desiccator

Chemical Reagents

  • Cement sample
  • Nitric acid, dilute (1+1)
  • Silver nitrate solution, 0.1 M
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 2.0 g of cement.
  2. Digest with 30 mL dilute HNO3 on a hot plate for 15 minutes.
  3. Filter off silica through quantitative paper; wash the residue.
  4. Dilute the filtrate to 200 mL in a foil-wrapped beaker and heat.
  5. Precipitate with AgNO3, digest warm, filter through a weighed sintered-glass crucible.
  6. Wash, dry at 150 C to constant mass and weigh AgCl; calculate % Cl.

Observations & Expected Results

Cement dissolves with effervescence; white AgCl precipitates from the filtrate. Typical mass 0.01-0.05 g from 2 g cement.

Worked Stoichiometric Calculations

Problem: 2.000 g of cement gave 0.0312 g AgCl. Calculate % Cl and comment on corrosion risk.

Working: Mass Cl = 0.0312 × 0.2473 = 0.007716 g. % Cl = (0.007716/2.000) × 100 = 0.386%. This is just below the commonly cited 0.40% corrosion threshold — borderline, and the cement should be used with caution in reinforced concrete.

Safety Precautions & Hazard Control

  • Use nitric acid for digestion; hydrochloric acid would contaminate the sample with chloride.
  • Remove silica fully before precipitation.
  • Protect AgCl from light.

Waste Disposal Protocol

Silver residues collected for recovery; acidic filtrates neutralised.

Viva Voce Oral Defense Questions & Answers

Q: Why is nitric acid used instead of hydrochloric acid to dissolve cement here?

A: HCl would introduce extraneous chloride and make the determination meaningless; HNO3 provides acidity without adding the analyte.

Q: Why is chloride in concrete a corrosion concern?

A: Chloride destroys the passive oxide film on steel reinforcement, initiating pitting corrosion that expands and cracks the concrete.

← Back to Experiments Directory