Silver in a Silver Alloy: Reverse AgCl Gravimetry

Determine silver in an alloy by dissolving it and precipitating Ag+ as AgCl.

Level: UniversitySafety: Advanced lab onlyTime: 2 h
Aim of Experiment: Determine silver in an alloy by dissolving it and precipitating Ag+ as AgCl.

Theoretical Foundations

The alloy is dissolved in nitric acid: 3Ag + 4HNO3 → 3AgNO3 + NO + 2H2O. Silver is then precipitated with chloride: Ag+ + Cl- → AgCl(s). This is reverse gravimetry — the analyte cation is precipitated by the anion. The gravimetric factor for silver is M_Ag/M_AgCl = 107.87/143.32 = 0.7527, conveniently large, giving a precise determination.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 250 mL beaker
  • Hot plate
  • Fume cupboard
  • Sintered-glass crucible
  • Oven
  • Desiccator

Chemical Reagents

  • Silver alloy sample
  • Nitric acid, concentrated and dilute
  • Sodium chloride solution, 10% w/v
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.4-0.5 g of alloy into a beaker.
  2. In a fume cupboard dissolve in 10 mL conc. HNO3 with gentle warming; evaporate to remove excess acid.
  3. Dilute to 200 mL, heat to near boiling in a foil-wrapped beaker.
  4. Add 10% NaCl solution dropwise with stirring until precipitation is complete.
  5. Digest warm, filter through a weighed sintered-glass crucible, wash with dilute HNO3.
  6. Dry at 150 C to constant mass and weigh AgCl.

Observations & Expected Results

Alloy dissolves with brown NO2 fumes; white AgCl precipitates on adding NaCl. Typical mass about 0.5 g from 0.5 g alloy.

Worked Stoichiometric Calculations

Problem: 0.5000 g of alloy gave 0.5215 g AgCl. Calculate % Ag. (GF_Ag = 0.7527)

Working: Mass Ag = 0.5215 × 0.7527 = 0.3925 g. % Ag = (0.3925/0.5000) × 100 = 78.51%.

Safety Precautions & Hazard Control

  • Dissolve in a fume cupboard; nitrogen oxides are toxic.
  • Protect AgCl from light throughout.
  • Ensure complete dissolution; undissolved metal gives low results.

Waste Disposal Protocol

Silver residues collected for recovery; acidic solutions neutralised.

Viva Voce Oral Defense Questions & Answers

Q: Why is this called reverse gravimetry?

A: The analyte is the cation (Ag+) precipitated by an anion (Cl-), the reverse of the usual anion-by-cation precipitation.

Q: Why is the gravimetric factor for Ag in AgCl favourable?

A: At 0.7527 it is large, so weighing errors in the precipitate translate into small relative errors in the silver result.