CHEMVEN

Acid-Soluble Sulfate in Portland Cement (Reported as SO3)

Determine the sulfate content of Portland cement, reported as % SO3 as in cement specifications.

Level: UniversitySafety: Needs supervisionTime: 3 h
Aim of Experiment: Determine the sulfate content of Portland cement, reported as % SO3 as in cement specifications.

Theoretical Foundations

Cement contains calcium sulfate (added as gypsum to control setting). Acid digestion dissolves the sulfate; silica is dehydrated and filtered off first so it does not contaminate the BaSO4. Precipitation: Ba2+ + SO4 2- → BaSO4(s). Cement results are conventionally reported as SO3 using the factor M_SO3/M_BaSO4 = 80.06/233.39 = 0.3430. Typical Portland cement contains 2-4% SO3.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 250 mL beaker
  • Hot plate
  • Quantitative filter paper
  • Ashless filter paper
  • Muffle furnace
  • Desiccator

Chemical Reagents

  • Portland cement sample
  • Hydrochloric acid, concentrated and dilute
  • Barium chloride solution, 10% w/v
  • Silver nitrate solution, 0.1 M
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 1.0 g of cement into a 250 mL beaker.
  2. Add 15 mL conc. HCl and 5 mL water; warm and stir until decomposition is complete.
  3. Evaporate to dryness on a hot plate to dehydrate silica; bake 1 hour at 110 C.
  4. Take up with 10 mL conc. HCl and 50 mL hot water; filter off silica through quantitative paper and wash.
  5. Dilute the filtrate to 200 mL, heat to boiling and precipitate with hot BaCl2.
  6. Digest 1 hour, filter, wash, ignite at 800 C to constant mass and weigh BaSO4.
  7. Calculate % SO3 = mass BaSO4 × 0.3430 × 100 / sample mass.

Observations & Expected Results

Cement effervesces in acid; a gelatinous silica residue remains on the first filter. White BaSO4 precipitates from the clear filtrate; typical mass 0.08-0.12 g per gram of cement.

Worked Stoichiometric Calculations

Problem: 1.0000 g of cement gave 0.0960 g BaSO4. Calculate % SO3.

Working: Mass SO3 = 0.0960 g × 0.3430 = 0.03293 g. % SO3 = (0.03293/1.0000) × 100 = 3.29%. (Within the usual 2-4% specification range.)

Safety Precautions & Hazard Control

  • Dehydrate silica fully or it passes through and contaminates the BaSO4.
  • Work in a fume cupboard when handling concentrated HCl.
  • Ignite to constant mass; cement filtrates contain much dissolved salt.

Waste Disposal Protocol

Acidic filtrates are neutralised before disposal; barium residues to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is sulfate in cement reported as SO3?

A: By long-standing convention in cement chemistry, all oxides are reported in oxide form (SiO2, Al2O3, SO3) for specification and Bogue calculations.

Q: Why must silica be removed before precipitating BaSO4?

A: Gelatinous silicic acid would coprecipitate with and contaminate the BaSO4, giving high, non-stoichiometric results.

Q: Why is gypsum added to cement?

A: To retard the setting time by controlling the hydration of tricalcium aluminate.