Determine total sulfur in a pyrite ore by oxidation of sulfide to sulfate followed by BaSO4 gravimetry.

Level: UniversitySafety: Advanced lab onlyTime: 3 h
Aim of Experiment: Determine total sulfur in a pyrite ore by oxidation of sulfide to sulfate followed by BaSO4 gravimetry.

Theoretical Foundations

Sulfide sulfur cannot be precipitated directly, so it is first oxidised to sulfate with bromine water or nitric acid: S2 2- → 2 SO4 2- (overall oxidation). Excess oxidant is removed by evaporation with HCl. The sulfate is then precipitated as BaSO4: Ba2+ + SO4 2- → BaSO4(s). The gravimetric factor for sulfur is M_S / M_BaSO4 = 32.06 / 233.39 = 0.1374.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 250 mL beakers with watch glasses
  • Hot plate
  • Ashless filter paper
  • Muffle furnace
  • Desiccator
  • Fume cupboard

Chemical Reagents

  • Pyrite ore sample, finely ground
  • Bromine water (saturated) or concentrated HNO3
  • Hydrochloric acid, concentrated
  • Barium chloride solution, 10% w/v
  • Silver nitrate solution, 0.1 M
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.4-0.5 g of finely powdered ore into a 250 mL beaker.
  2. In a fume cupboard add 20 mL bromine water (or 15 mL conc. HNO3), cover and warm gently until the dark particles dissolve.
  3. Add 5 mL conc. HCl and evaporate to near dryness to remove excess oxidant and nitrates; repeat with 5 mL HCl.
  4. Dissolve the residue in 200 mL hot water with 1 mL dilute HCl and filter off insoluble gangue.
  5. Heat the filtrate to boiling and precipitate sulfate with hot 10% BaCl2 added dropwise.
  6. Digest 1 hour, filter, wash chloride-free, ignite at 800 C to constant mass and weigh BaSO4.

Observations & Expected Results

Dark ore particles dissolve giving a yellow-brown solution that becomes pale after evaporation. A heavy white BaSO4 precipitate forms; typical mass 1.2-1.5 g from 0.5 g ore.

Worked Stoichiometric Calculations

Problem: 0.5000 g of pyrite ore gave 1.3520 g BaSO4. Calculate % S in the ore. (GF for S = 0.1374)

Working: Mass of S = 1.3520 g × 0.1374 = 0.1858 g. % S = (0.1858 / 0.5000) × 100 = 37.15%. (Pure FeS2 contains 53.45% S; the ore is lower grade.)

Safety Precautions & Hazard Control

  • Work in a fume cupboard: bromine vapour and nitrogen oxides are toxic.
  • Oxidation must be complete; undissolved dark particles mean low results.
  • Remove all nitrate before precipitation or Ba(NO3)2 will coprecipitate.
  • Evaporate with HCl twice to expel oxidising gases fully.

Waste Disposal Protocol

Acidic bromine/nitrate filtrates are neutralised before disposal; barium residues go to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why must sulfide be oxidised before precipitation?

A: Sulfide does not form a stoichiometric weighable precipitate with Ba2+ (BaS is soluble); oxidation to sulfate gives the insoluble, stoichiometric BaSO4.

Q: Why evaporate with HCl after oxidation?

A: To destroy excess bromine/HNO3; residual nitrate causes coprecipitation of Ba(NO3)2 and high results.

Q: What is the gravimetric factor for sulfur in BaSO4 and how is it derived?

A: M_S / M_BaSO4 = 32.06 / 233.39 = 0.1374; one mole of BaSO4 contains one mole of S atoms.